Heat Treat Specifications

Superior Chisel Steel Analysis
    Carbon .55 -.60
    Manganese .70 -.90
    Silicon 1.80 - 2.20
    Chrome .20 - .35
    Moly .15 - .25
  Heat Treat Spec. For Above Steel
  Start Forge 1800o - 2000oF - Stop
    Forge @ 1500oF (Cherry Red)
  Hardening:
    Heat to 1625oF & Quench in Oil
    Draw to 650oF
    Rockwell "C" 48-52
    Decarb. will be .010 - .020
     
  If standard heat treating furnaces are not available, use the color system - the chisel should be heated to a light orange color and to be quenched in oil.
 
 